1. Properties
1. Wide technique range and good covering ability. The throwing power can increase by 30~60%, the current efficiency is up to 22~24%, non-corrosion at the low current area.
2. HV hardness increases by 10~30%, the period of neutral salt-spraying test increases 1~2 times.
3. Low content of chromic acid, it is 40% of routine plating solution, lower the content of chromic acid in waste water, easy to be treated, high economic efficiency.
4. The technique is stable, easy to maintain.
2. Technical Formulation and Operating Condition
Chromic acid (CrO3) |
140~180 g/L |
Sulfuric acid (H2SO4) |
0.4~1 g/L |
WR-1 |
1~2 g/L |
Cr3+ |
< 4 g/L |
Temperature |
25~70℃ |
DK |
5~60 A/dm2 |
Anode |
Lead-Tin alloy plate (Tin content 8~15%) |
Sk : SA |
1:3 below |