Nickel BP 760 Barrel Nickel Plating Additive
Properties
1. Good leveling performance, good covering power.
2. The plating layer can be with low stress, excellent flexibility. It is suitable for machining parts after plating.
3. Wide range electric current density and additive replenishment, stable bath and easy to control.
Formula and Operation Condition |
Range |
Nickel Sulfate (NiSO4·7H2O) |
180~250g/L |
Nickel Chloride (NiCl2·6H2O) |
45~55g/L |
Boric Acid (H3BO3) |
40~50g/L |
Nickel BP 760A brightener |
0.2~0.4ml/L |
Nickel BP 760B softener |
6~10ml/L |
Y1 wetting agent |
1~2ml/L |
PH |
3.8~4.5 |
Temperature |
50~65℃ |
Cathode Current Density |
2.5~8.0A/dm2 |
Anodic Current Density |
1.0~3.0A/dm2 |
Filtration |
Recycle filteration continuously |
Nickel Plating Additive Consumption
Additive |
Consumption |
Nickel BP 760A brightener |
100~250ml/KAh |
Nickel BP 760B softener |
100~225ml/KAh |
Y1 wetting agent |
20~50ml/KAh |