EN-100 Acid Electroless Nickel
This process can reduce the nickel phosphorus alloy coating on the workpiece through the non electrolytic self catalytic reaction of the solution. The coating has the characteristics of uniform thickness, excellent corrosion resistance, good wear resistance, high brightness, and high hardness. The plating solution has good stability, strong impurity resistance, and easy adjustment. This product can be used for chemical nickel deposition on metal and non-metal parts of various shapes.
I. Coating Characteristics
- The phosphorus content is (10.0-14.0)%;
- Hardness (500-600) HV, can reach (900-1000) HV after heat treatment;
- The maximum sedimentation rate can reach 10-20 micrometers per hour.
II. Preparation of Plating Solution
| Composition and operating conditions |
Process Parameters |
| EN-100 A |
60 ml |
| EN-100 B |
160 ml |
| pH |
4.5 - 5.5 |
| Temperature |
85 - 90 ℃ |
| Working load capacity |
0.2-2 dm²/L |
| Agitation or stirring |
Air agitation for filtration |